Independent thesis Advanced level (degree of Master (Two Years)), 20 credits / 30 HE credits
Bone tissue engineering scaffolds must combine mechanical competence with a surface chemistry capable of supporting cell attachment and osteogenesis, a combination unmodified poly(lactic acid) (PLA) does not provide. This study fabricated PLA/Laponite nanocomposite fibres by melt spinning, a solvent-free and industrially scalable route, to evaluate whether incorporating Laponite, a synthetic layered silicate nanoclay, can reinforce the PLA matrix while introducing a bioactive, ion-releasing phase.
Formulations containing 0.5, 1, 5, and 10 wt% Laponite were melt compounded, converted into continuous filaments by piston melt spinning, and drawn uniaxially at draw ratios of 3, 4, and 5.
Processability, chemical structure, thermal behaviour, fibre morphology, and mechanical performance were evaluated by Fourier-transform infrared spectroscopy (FTIR), differential scanning calorimetry (DSC), thermogravimetric analysis (TGA), optical microscopy, and uniaxial tensile testing. Laponite loadings of 0.5-5 wt% were compatible with stable filament formation; 10 wt% was not melt-spinnable under the conditions used.
Tensile testing (n = 10 per formulation, one-way ANOVA with Tukey HSD, p < 0.001) identified 1 wt% Laponite drawn to a ratio of 4 as the formulation with the highest tenacity and load-bearing capacity, consistent with a synergistic interaction between nanoclay reinforcement and draw-induced molecular orientation.
DSC indicated that Laponite acts principally as a heterogeneous nucleating agent, lowering the cold-crystallisation temperature at every loading tested. TGA confirmed loading-dependent retention of Laponite within the fibre (residual char rising from 0.99 ± 0.14% for neat PLA to 5.49 ± 0.39% at 10 wt%) without a statistically significant shift in decomposition onset.
Optical microscopy showed uniform Laponite dispersion at 1 wt% and progressive agglomeration at 5 wt%, consistent with the loss of mechanical reinforcement and processability above this loading.
These physicochemical results indicate that Laponite is retained within the melt-spun PLA fibre in a form consistent with the capacity for hydrolytic ion release reported for Laponite elsewhere in the literature, and that 1 wt% Laponite processed to a draw ratio of 4 offers the best-balanced combination of dispersion quality, thermal nucleation behaviour, and mechanical reinforcement identified in this study.
No cell-culture, ion-release, or rheological data were generated, so bio-integration potential is not demonstrated here; it is a structurally motivated hypothesis for future testing.
This composition is proposed as the lead candidate for the hydrolytic degradation and biological evaluation studies required before the scaffold's suitability for bone tissue engineering can be assessed.
2026.
poly(lactic acid), Laponite nanoclay, melt spinning, nanocomposite fibres, heterogeneous nucleation, strain-induced crystallisation, bone tissue engineering